A narrow line on a new impeller casting invites a quick label: scratch, parting mark, cold shut. Those labels describe different things. Before anyone blends the line away, separate what is visible from what has actually been established about the metal.
A cold shut in investment casting concerns incomplete bonding where metal fronts meet. The important question is continuity at that interface, not simply whether the surface looks tidy.
Start with the line, not the assumed cause
Record the line's path on the component: the vane side or shroud face, its beginning and end, and any change around an edge. Keep a wider view showing its location alongside the close-up. “A line near the outlet” is a more useful observation than a tightly cropped image labeled “cold shut.”
The ICI cold-shut atlas entry describes the meeting of incompletely bonded metal fronts and identifies thin sections and areas distant from the gate among typical locations. Those locations guide investigation; they do not turn every line there into the same defect.
A pattern line and a metal interface answer different questions
A line can originate before metal is poured. ICI's wax-pattern atlas, under Flow Lines / Knit Lines, documents pattern-stage line features. The cold-shut atlas identifies wax knit lines as a similar appearance that needs to be distinguished from metal non-bonding.
The distinction is between a surface form inherited from an earlier stage and a failure of the metal fronts to join. These explanations cannot be exchanged simply because a photograph shows a narrow line. Nor does the word “casting” establish when the line first appeared.

Choose evidence that reaches the question
Visual examination records the feature. Penetrant examination can reveal an indication open to the tested surface. A section examined metallographically can investigate the material through a suspected interface. ICI includes these methods in its cold-shut investigation guidance; they are not interchangeable guarantees.
For example, a penetrant indication does not by itself explain when the feature formed. A clean-looking surface after grinding does not show the condition below that new surface. Use the penetrant-versus-radiographic inspection guide to keep a report's coverage separate from the component's full acceptance requirements.
Preserve the original observation before further surface work. Additional blending changes the feature available to the next reviewer. If the original line, location and processing stage were not recorded, a later photograph of a smoother patch cannot reconstruct them.
This is a different investigation from pores exposed during machining. A line-shaped indication should not inherit the same cause or disposition merely because both were found on a bronze casting.
For a new impeller manufacturing enquiry, use the pump impeller casting page and identify any drawing-defined inspection region or acceptance requirement with the affected feature. Keep that requirement separate from a photo-based defect label so the requested evidence addresses the actual component question.